Welding Defects

Any irregularity (discontinuity or flaw) in the weld metal, which exceeds the applicable code limit, is termed as a WELD DEFECT (or Welding Defect). Please note that a discontinuity can be termed as a defect only when, if it exceeds the specified code limit, hence we can say that every defect present in a weld metal is a discontinuity but every discontinuity present in the weld metal may not necessarily be a defect. A defect can be macroscopic or microscopic.

Defects may occur due to the following reasons;

1. Incorrect welding parameters
2. Inappropriate welding procedures
3. Poor process condition
4. Inappropriate selection of filler metal and parent metal
5. Unskilled welder or welding operator
6. Incorrect job preparations

Classification of Defects:

Defects can be classified as external defect (also known as visual defect or surface defect) and internal defect (also known as hidden defect or subsurface defect). External defects are those which are found on the surface itself. Internal defects are those which exist in the material at some depth. We can say that defects which are not present on the surface are internal defects. Please see the following table;

classification of weld defects

 

1. CRACKS: It is the most dangerous of all defects. Cracks may be of any size or shape; it can be either microscopic or macroscopic. Cracks may appear anywhere i.e. on the surface, subsurface, at any depth or at the root. Crack occurs when the localized stress exceeds the ultimate Tensile Stress (UTS) of the material. It may propagate within the material.

Crack - Welding defect

Cracks are of two types;

  • Hot Crack
  • Cold Crack

HOT CRACK: Hot cracks occurs during welding or soon after completion of welding, It is most likely to occur during the solidification of the molten weld pool. Hot cracks mostly occur in the weld metal but it may occur at the Heat Affected Zone (HAZ) region too.

When hot crack occurs on the weld metal then it is termed as Solidification Crack and if it occurs in the HAZ then called as Liquation crack.

Causes of Hot Crack:
1. High concentration of residual stress
2. Rapid cooling of weld pool
3. High thickness of base material
4. Poor ductility of welded material
5. High welding current
6. Inadequate heat treatment

Prevention:
1. Preheating and post heating to avoid rapid cooling
2. Using right filler metal

COLD CRACK: Cold cracks occur after the solidification of weld metal; it can even develop several days after completion of welding. Most of the time it develops in the HAZ but may occur on the weld metal too. It is often associated with non-metallic inclusion.

Causes of Cold Crack:

1. Diffusion of Hydrogen atoms: Hydrogen atoms cause cold cracking. These hydrogen atoms may be induced in the weld metal from the surrounding, electrode, base metal or any contamination present on the root face.

2. Lack of Preheating: Due to inadequate preheating, microstructural changes may take place. Microstructural crystals may re-structure itself to form martensite. Matensite is very prone to cracks. Preheating also helps in reducing diffusion of hydrogen atoms and ensures no moisture on the joint before welding.

Prevention:
1. Preheating and post welding the weld metal
2. Using low Hydrogen electrode

STAR CRACK (CRATER CRACK): Star crack is a type of hot crack and it develops at the crater on the weld metal. A crater is a depression formed on the weld bead where arc gets broken or when electrode is changed.
It develops when center of the weld pool solidifies before its surrounding and due to this the center pulls the outer weld and thus star cracks are formed.

2. POROSITY/BLOW HOLES: Porosity is a small pore or void whereas blowholes are comparatively larger hole or cavity. It may be present on the surface or inside the weld metal. Porosity can occur individually or it may occur in groups also (mostly), group of porosity is known as cluster porosity.

Porosity - Welding Defect

Causes of Porosity:

Porosity occurs due to the entrapment of gases in the molten weld pool, these entrapped gases doesn’t get a chance to release and hence causes porosity or blowhole. Gases which are entrapped are mostly Hydrogen, Carbon mono oxide, Carbon dioxide, Nitrogen and Oxygen. Source of these gases are fluxes present on the welding electrode, Moisture, Oil, Grease other foreign contaminants present on the joint etc.

Prevention:

  1. Use low Hydrogen electrode
  2. Baking of electrodes before welding as per the recommended procedure
  3. Through cleaning of joint surface and adjacent area before welding
  4. Preheat the joint before welding
  5. Ensure sufficient flow of shielding gases if using TIG or MIG welding

3. UNDERCUT: Undercut appears as a narrow groove on the base metal adjacent to the weld metal along the edge. Undercut always runs parallel to the weld metal. It acts as a stress raiser during fatigue loading.

Undercut - Welding Defect

Causes of Undercut:
1. High welding current and arc voltage
2. Large electrode diameter
3. Incorrect electrode angle
4. Longer arc length

4. UNDERFILL: When the weld metal surface remains below the adjacent surface of the base metal then it is called as an underfill. Underfill is an undersized welding.

Underfill - Welding Defect

5. LACK OF PENETRATION: When the weld metal doesn’t completely penetrate the joint, then it is called as Lack of Penetration of Incomplete Penetration. It is one of the most dangerous defects, since it acts as a stress raiser and hence crack may originate or propagate from here.

Lack of penetration (LOP) or Incomplete penetration (IP) - Welding Defect

Causes of Lack of Penetration:
1. Root gap too small
2. Fast travel speed
3. Low heat input
4. Too large an electrode diameter

Prevention:
1. Proper joint preparation i.e. providing a suitable root gap.
2. Proper heat input
3. Correct travel speed
4. Using electrode of suitable size

Lack of penetration can be repaired by proper back gouging.

6. LACK OF FUSION: It is the lack of proper melting (or proper fusion) either between the weld metal with the base metal or one layer of the weld with the other layer. Lack of fusion is also called as Cold lapping or cold shuts. One of the most prominent reasons for the cause of lack of fusion is poor welding technique. Lack of fusion is an internal defect, but it can occur on the external surface too, if the sidewall of parent metal doesn’t get properly fused with the base metal, as shown in the below figure and for this case lack of fusion can also be called as ‘lack of sidewall fusion’.

Lack of fusion or incomplete fusion (LOF or IF) - Welding Defect

Causes of Lack of Fusion:
1. Low welding current
2. Travel speed to high or too low
3. Unfavorable heat input

7. SPATTERS: Spatters are small globular metal droplets (of weld metal) splashed out on the base metal during welding. Spatters stick on the base metal hence can be removed by wire brush or buffing.

Spatters - Welding Defect

Causes of Spatters:
1. Excessive arc current
2. Excessive long arc
3. Improper shielding gases
4. Electrode with improper flux
5. Damp electrodes

8. OVERLAP: Overlap occurs due to the overflow of weld metal on the surface of base metal. During welding, molten metal overflows on the base metal without fusing with the base metal.

Overlap - Welding Defect

Causes of Overlap:
1. Current too low
2. Large deposition in a single run
3. Longer arc
4. Slow arc travel speed

9. EXCESSIVE PENETRATION: When the penetration of weld metal is too high through the joints then it is called as excessive penetration. It acts as notch where stress concentration takes place. In addition to this it results in economical wastage.

Excess Penetration - Welding Defect

Causes of Excessive Penetration:
1. Too wide a root gap
2. High welding current
3. Slow travel Speed

10. INCLUSION: Entrapment of any foreign material (either metallic or non metallic) in the weld metal is called as inclusion. If slag doesn’t get a chance to float over the surface of molten weld pool, then it gets entrapped within the weld metal such inclusion is called as slag inclusion. Similarly, sometimes droplets of tungsten get entrapped within the weld metal resulting in tungsten inclusion (in TIG welding). Sulphides, oxides and silicates also get entrapped resulting in inclusion. Inclusion acts as a stress raiser hence should be avoided.

Inclusion - Welding Defect

11. WAGON TRACKS: Linear slag inclusion along the axis of the weld is called as wagon tracks. During root pass a groove is formed at the toe, due to wrong welding techniques, and that groove is filled by slag (especially Hydrogen which has been trapped by the solidified slag) and thus wagon tracks are formed. It is also known as worm tracking.

Wagon Tacks - Welding Defect

12. ARC STRIKE: When the electrode or the electrode holder, unintentionally or accidentally strikes with the work piece, an unwanted arc is generated causing arc strike. Arc strikes may initiate failure in bending and cyclic loading. In addition to this is affects the aesthetics of the work piece.

13. SHRINKAGE CAVITY: During solidification of the molten weld pool, metal shrinkage occurs. Due to the shrinkage of weld metal a cavity is formed known as shrinkage cavity.

Please click here, to read the acceptance/rejection criteria for weld defects.

Please watch this video lecture (given below) for a better understanding of welding defects: 

 

Sandeep Anand

I am a Mechanical Engineer with more than ten years of work experience in the field of welding and NDT.

15 thoughts on “Welding Defects

  • March 31, 2018 at 7:33 am
    Permalink

    One defect I never new the cause of. Worm hole porosity in FCAW welding. Can you comment ?

    Reply
    • March 31, 2018 at 3:56 pm
      Permalink

      Happens especially when on a T joint on side is welded already and you weld the other side and the gas gets trapped under the plate.

      Reply
  • April 1, 2018 at 11:43 am
    Permalink

    Thanks for basic information or welding

    Reply
  • April 1, 2018 at 5:23 pm
    Permalink

    Wagontracks should be parallel lines. What is depicted is an ElongatedvSlag Inclusion (ESI)

    Reply
  • April 8, 2018 at 4:05 pm
    Permalink

    Super demonstration

    Reply
  • June 11, 2018 at 9:27 am
    Permalink

    Thanks for valuable Basic Information with Remedies

    Reply
  • June 11, 2018 at 9:38 pm
    Permalink

    Excellent work, great demonstration

    Reply
  • June 12, 2018 at 2:08 am
    Permalink

    In my personal experience the main cause of porosity are the air currents in smaw and gmaw process

    Reply
  • October 23, 2018 at 12:27 pm
    Permalink

    Thanks sir for the valuable information about welding defects

    Reply
  • November 4, 2018 at 6:43 am
    Permalink

    Porosity came in ss welding by 309l what to do?

    Reply
  • May 2, 2019 at 8:19 am
    Permalink

    Thanks and i appreciate for this explanation about Defects.

    Reply
  • August 28, 2019 at 5:05 am
    Permalink

    Explainations were made easier to remember and valuable thankq sir

    Reply
  • September 9, 2019 at 1:23 pm
    Permalink

    Weld spatter is not considered a weld defect according ISO-5817, acceptance depends on application so if not specific specified weld spatter is not an rejection criteria

    Reply

Leave a Reply

Your email address will not be published. Required fields are marked *